Stick Electrodes Low Alloy Steel Welding Rod AWS E8011-G with High Cellulose Potassium Coating

Short Description:

J555 (AWS E8011-G) is a vertical downward electrode with high cellulose potassium coating. AC and DC dual-purpose.


Product Detail

Product Tags

J555                                                       

GB/T E5511-G  

AWS E8011-G                                

Description: J555 is a vertical downward electrode with high cellulose potassium coating. AC and DC dual-purpose. when welding downward, molten metal and slag will not flow down. It has great arc force and penetration. Bottom welding can be formed on both sides and has high welding speed.

Application: Used for welding low alloy steel pipes.

Chemical composition of weld metal(%):

C

Mn

Si

S

P

≤0.20

≥1.00

≤0.50

≤0.035

≤0.035

 

Mechanical properties of weld metal:

Test item

Tensile strength

Mpa

Yield strength

Mpa

Elongation

%

Impact value (J)

-30℃

Guaranteed

≥540

≥440

≥17

≥27

X-ray inspection:  II grade

 

Recommended current:

(mm)

Rod diameter

2.5

3.2

4.0

5.0

(A)

Welding Current

45 ~ 75

80 ~ 120

130 ~ 160

170 ~ 190

 

Notice:

The electrode must be baked at 70-90°C for 1 hour before use. The temperature should not be too high, otherwise the cellulose in the coating will be damaged.

 

Wenzhou Tianyu Electronic Co., Ltd. was established in 2000. We have been engaged in the manufacturing of welding electrodes, welding rods, and welding consumables for more than 20 years.

Our main products include stainless steel welding electrodes, carbon steel welding electrodes, low alloy welding electrodes, surfacing welding electrodes, nickel & cobalt alloy welding electrodes, mild steel & low alloy welding wires, stainless steel welding wires, gas-shielded flux cored wires, aluminum welding wires, submerged arc welding. wires, nickel & cobalt alloy welding wires, brass welding wires, TIG & MIG welding wires, tungsten electrodes, carbon gouging electrodes, and other welding accessories & consumables.

 


  • Previous: